ISO 13500:2008(en) Petroleum and natural gas industries — Drilling fluid materials — Specifications and tests
ISO 13500:2008(en) Petroleum and natural gas industries — Drilling fluid materials — Specifications and tests
Foreword
This third edition cancels and replaces the second edition (ISO 13500:2006), subclauses 7.1.2/Table 2, 7.3.1, 8.5.2, 8.6.5, 8.13.4, 10.2.5, 11.4, 14.4.3, and 15.4.3 of which have been technically revised. Clause 17 on low-viscosity polyanionic cellulose, Clause 18 on high-viscosity polyanionic cellulose, and Clause 19 on drilling-grade xanthan gum have been added.
Introduction
Annex A (informative) lists the mineral impurities in barite, Annex B (informative) provides the test precision and Annex C (informative) details examples of calculations.
1 Scope
This International Standard covers physical properties and test procedures for materials manufactured for use in oil- and gas-well drilling fluids. The materials covered are barite, haematite, bentonite, nontreated bentonite, OCMA-grade bentonite, attapulgite, sepiolite, technical-grade low-viscosity carboxymethylcellulose (CMC-LVT), technical-grade high-viscosity carboxymethylcellulose (CMC-HVT), starch, low-viscosity polyanionic cellulose (PAC-LV), high-viscosity polyanionic cellulose (PAC-HV) and drilling-grade Xanthomonas campestris (Xanthan gum). This International Standard is intended for the use of manufacturers of named products.
2 Normative references
ISO 6780, Flat pallets for intercontinental materials handling — Principal dimensions and tolerances
ISO 10414-1:2008, Petroleum and natural gas industries — Field testing of drilling fluids — Part 1: Water-based fluids
ASTM D422, Standard Test Method for Particle-Size Analysis of Soils
ASTM E11, Standard Specification for Wire Cloth and Sieves for Testing Purposes
ASTM E161, Standard Specification for Precision Electroformed Sieves
ASTM E77, Standard Test Method for Inspection and Verification of Thermometers
ASTM E177, Standard Practice for Use of the Terms Precision and Bias in ASTM Test Methods
NIST (NBS) Monograph 150, Liquid-In-Glass Thermometry
3 Terms, definitions, symbols and abbreviations
3.1 Terms and definitions
side containing residue (“flash”) from stamping, or the side with concave indentation
3.2 Symbols and abbreviations
ACS | American Chemical Society |
API | American Petroleum Institute |
APME | Association of Plastic Manufacturers in Europe |
ASTM | American Society for Testing and Materials |
EDTA | Ethylenediaminetetraacetic acid |
CAS | Chemical Abstracts Service |
CMC-HVT | Carboxymethylcellulose — High-viscosity, technical-grade |
CMC-LVT | Carboxymethylcellulose — Low-viscosity, technical-grade |
OCMA | Oil Companies' Materials Association |
NBS | National Bureau of Standards |
NIST | National Institute of Standards and Technology |
TC | to contain |
TD | to deliver |
Bc | hydrometer correction curve intercept |
b | yield point/plastic viscosity ratio |
D1 | equivalent particle diameter immediately greater than 6 µm, determined in Equation (9) |
D2 | equivalent particle diameter immediately less than 6 µm, determined in Equation (9) |
De | equivalent spherical diameter, expressed in micrometres |
Cc | calibration correction |
Cm | 40 times the EDTA volume, expressed in millilitres |
KS | sample constant |
L | effective depth, expressed in centimetres |
log(η20/ηθ) | correction for temperature variance |
Mc | hydrometer correction curve slope |
m | sample mass, expressed in grams |
m2 | residue mass, expressed in grams |
m3 | mass of the 425 µm sieve, expressed in grams |
m4 | mass of 425 µm sieve and sample retained, expressed in grams |
m5 | mass passing through a 425 µm sieve, expressed in grams |
m6 | mass of the bottom receiver, expressed in grams |
m7 | mass of the bottom receiver and sample content, expressed in grams |
m8 | mass of sample passing through a 75 µm sieve, expressed in grams |
R | hydrometer reading |
R1 | average hydrometer reading at lower temperature |
R2 | average hydrometer reading at higher temperature |
R600 | viscometer dial reading at 600 r/min |
R300 | viscometer dial reading at 300 r/min |
Ss | sample test value |
t | time, expressed in minutes |
V | total filtrate volume, expressed in millilitres |
Vc | filtrate volume, expressed in millilitres, collected between 7,5 min and 30 min |
V1 | initial volume, expressed in millilitres |
V2 | final volume, expressed in millilitres |
V3 | volume EDTA used, expressed in millilitres |
V4 | volume of filtrate used, expressed in millilitres |
w1 | mass fraction residue of particles greater than 75 µm, expressed in percent |
w2 | cumulative percent for point immediately greater than 6 µm |
w3 | cumulative percent for point immediately less than 6 µm |
w4 | cumulative percent less than 6 µm |
w5 | mass fraction residue of particles greater than 45 µm, expressed in percent (see 8.9.6) |
w6 | mass fraction moisture, expressed in percent |
wa | cumulative percent finer |
wAEM | soluble alkaline earth metals as calcium, expressed in milligrams per kilogram |
w75 | mass fraction of sample passing through a 75 µm sieve, expressed in percent |
w425 | mass fraction passing through a 425 µm sieve, expressed in percent |
ρ | sample density, expressed in grams per millilitre |
θ | temperature, expressed in degrees Celsius or degrees Fahrenheit |
θ1 | average temperature reading at lower temperature |
θ2 | average temperature reading at higher temperature |
ηA | apparent viscosity, expressed in centipoise |
η | viscosity of water, expressed in millipascal seconds |
η20 | 1,002, is the viscosity of water at 20 °C (68 °F) |
ηθ | viscosity at desired temperature (see Table 3) |
ηP | plastic viscosity, expressed in millipascal·seconds |
ηY | yield point, expressed in pounds per 100 ft2 |
Bibliography
[1] | ISO 31 (all parts), Quantities and units |
[2] | ISO 3310-1, Test sieves — Technical requirements and testing — Part 1: Test sieves of metal wire cloth |
[3] | ISO 10241, International terminology standards — Preparation and layout |
[4] | API RP 13K, Recommended Practice for Chemical Analysis of Barite |
[5] | ASTM E691, Standard Practice for Conducting an Interlaboratory Study to Determine the Precision of a Test Method |
[6] | API Spec 13A, Specification for Drilling-Fluid Materials, 16th Edition, February 1, 2004 |
[7] | API 88-30, 1989. Specification Parameters Determination Drilling Fluid Materials |
[8] | API 89-30, 1990. Specification Parameters Determination Drilling Fluid Materials |
[9] | API 90-30, 1992. Specification Parameters Determination Drilling Fluid Materials |
[10] | Korosi, A. and Fabuss, B. Analytical Chemistry, Vol 40 No. 1, Jan. 1968, “Viscosity of Liquid Water from 25 °C to 150 °C”, p. 162 |
Made in China Mao Qun stainless steel wire mesh, stainless steel screen mesh, stainless steel woven mesh, nickel alloy wire mesh, copper wire mesh, screen mesh,GFW metal wire mesh,Stainless steel wire mesh,Alloy wire mesh,Knitted metal wire mesh,Woven Wire Mesh,Structured packing